Formulation verification study results for Tank 106-AN waste
Author(s) -
R.O. Lokken
Publication year - 1992
Language(s) - English
Resource type - Reports
DOI - 10.2172/479173
Subject(s) - ground granulated blast furnace slag , fly ash , grout , cement , slag (welding) , portland cement , waste management , environmental science , materials science , metallurgy , composite material , engineering
Because of the excessive heat generated during hydration of double- shell tank waste grouts using 47 wt% blast furnace slag/47 wt% class F fly ash/6 wt% type I/II Portland cement, a modified formulation was recommended for testing of Tank 106-AN grout. The recommended dry blend is: 40 wt% agricultural grade CaCO{sub 3} (ground limestone), 28 wt% blast furnace slag, 28 wt% class F fly ash, and 4 wt% type I/II cement. Verification studies with this dry blend showed that the only criterion not met in all cases was for drainable liquid